    TCB-100A Bright Super-Black Ink of High Dyne Level

    來源: 發布時間:2019-04-17

     

    This printing ink, meeting the high requirements of the touch screen industry, is two component bright super-black insulation glass ink. The cured film has various advantages, such as good adhesion, water resistance, chemoresistance, printability, surface hardness and abradability.

    Operation process: Add 12 portions of the TCB-100B hardener into 100 portions of this ink and dilute the mixture, then print with the 300-420 mesh halftone.

         First coating: Baking at 160℃ for 10min;        Second coating: Baking at 160℃ for 20min.

    Technichal parameters are shown in the following table.

    Test Items

    Test Methods

    Test Tools

    Evaluation Criteria

    Test Results

    Fineness

    GB/T1724-79

    25μm Scraper fineness meter

    5μm

    5μm

    Surface tension

    Application criterion of the dyne pen

    Standard dyne pens

    30

    30dyn/cm

    Size change

    Quadratic element measuring instrument standard manufacture procedure (165S, 420 mesh printing)

    Quadratic element measuring instrument

    40μm

    26μm

    Ultrasonic washing

    Ordinary detergent, 65, 2hr

    Ultrasonic oscillating instrument, cross-cut tester, 3M gummed paper

    Non-foaming;non-wrinkling; non-discoloring;cross-cut adhesion test, 100%

    5B

    Boiling resistance

    Soaking in 100 deionized water for two hours

    Water bath

    Non-foaming;non-wrinkling; non-discoloring;cross-cut adhesion test, 100%

    5B

    High and low temperature humidity and heat cycle

    80, 95% RH (8hr); -20(2hr); ten cycles in total

    Test chamber

    Non-foaming;non-wrinkling; non-discoloring;cross-cut adhesion test, 100%

    5B

    Hardness

    Mitsubishi Pencil at an angle of 45 degrees, 500-gram force, measuring at different locations for 3 times

    Hardness tester, Mitsubishi Pencil

    3H

    3H

    Adhesion

    Cutting 100 grids, 3M gummed paper, continuously pulling off for 5 times

    cross-cut tester, 3M gummed paper

    cross-cut adhesion test, 100%

    3H

    Surface resistance

    Testing surface resistance at 5 locations (≤80%RH)

    Surface Resistance Tester

    1010Ohm

    ≥1010Ohm

    Acid resistance

    Soaking in 25 5% H2SO4 solution for two hours

    Thermostatic water bath, glassware

    Non-foaming;non-wrinkling;non-discoloring;cross-cut adhesion test, 100%

    5B

    Alkali resistance

    Soaking in 25 5% NaOH solution for two hours

    Thermostatic water bath, stainless steel ware

    Non-foaming;non-wrinkling; non-discoloring;cross-cut adhesion test, 100%

    5B

    Ethanol tolerance

    Tester loaded with 200 grams; using the winsey, dipped with over 99% alcohol, to rub back and forth for 100 times

    Low belt friction machine, winsey, alcohol

    Colorfast; not tarnishing

    Qualified

    Solvent (Acetone) resistance

    Tester loaded with 200 grams; using the winsey, dipped with chemically pure acetone, to rub back and forth for 50 times

    Low belt friction machine, winsey, acetone

    Colorfast; not tarnishing

    Qualified

     1. Performance features:

    Its obvious predominance lies in environmental compliance, no irritative odor, excellent blackness, good thixotropic structure and

    medium drying speed. 

    2. Usage:

    1) Before use, add the matched TCB-100B hardener (in the proportion of 12%) and moderate thinner into the ink and then fully 

      stir the mixture before printing. 

        2) The recommended baking temperature is 160℃ and the recommended baking time is 10-15min. On other conditions, please 

          confirm the feasibility in advance in order not to affect the product quality. 

    3) During the multilayer overprint, in order to ensure the quality, the first coating solidifies after baking at 160℃ for 10min; the 

      second coating solidifies after baking at 160℃ for 20min.

    4) The selection of the thinner types and the thinner dosage depend entirely on the adjustment of printing mesh number, 

      environmental condition and printing effect.

    3. Storage condition:

      Before and after using this series of ink, the ink containers should be kept completely sealed in cool and ventilated places to avoid 

      exposure to open fire and high temperature. 

    4. Guarantee period:

      The guarantee period is one year since the production date. Beyond the deadline, please reconfirm the usability.

    Note 1: All the above tolerance test data, derived from our test results, is for your reference only and not listed as guarantee value.

    Note 2: This series of ink meets the standard of RoHS2.0, REACH, Halogen and all of the test data concerning eight heavy metals.

     

    亚洲av无码一区二区三区四区| 亚洲欧洲无码AV不卡在线| 国产精品亚洲片在线花蝴蝶| 亚洲 欧洲 日韩 综合在线| 亚洲理论在线观看| 亚洲欧洲中文日产| 亚洲免费网站在线观看| 亚洲伊人久久精品| 亚洲一区电影在线观看| 亚洲人成电影在线观看青青| 亚洲国产午夜电影在线入口| 久久精品国产亚洲av麻豆蜜芽| 亚洲日韩乱码中文无码蜜桃臀| 亚洲成在人线中文字幕| 亚洲一级毛片在线观| 麻豆狠色伊人亚洲综合网站| 亚洲性线免费观看视频成熟 | 精品久久亚洲中文无码| 国产婷婷综合丁香亚洲欧洲| 亚洲综合久久精品无码色欲| 亚洲色最新高清av网站| 亚洲欧洲AV无码专区| 亚洲av无码一区二区三区人妖 | 亚洲AV无码无限在线观看不卡| 在线观看日本亚洲一区| 亚洲精品久久久久无码AV片软件| 噜噜综合亚洲AV中文无码| 亚洲国产成人VA在线观看| 中文国产成人精品久久亚洲精品AⅤ无码精品 | 亚洲精品第一国产综合亚AV| 日韩国产精品亚洲а∨天堂免| 亚洲?V乱码久久精品蜜桃| 久久久久噜噜噜亚洲熟女综合 | 亚洲国产成+人+综合| 亚洲小说图区综合在线| 国产成人亚洲精品播放器下载| 亚洲国产中文字幕在线观看 | 伊人久久亚洲综合影院首页| 国产精品观看在线亚洲人成网| 精品国产亚洲男女在线线电影| 亚洲αv在线精品糸列|